產(chǎn)品詳細(xì)介紹 |
項(xiàng) 目 \ 牌 號 |
NZ-82 |
TP |
N2 |
CN-45 |
ASC-T |
ASC-Z |
ASC-D |
ASC-SD-T |
ASC-SD-Z |
ASC-SD-D |
ASC-H |
ASC-L |
Al2O3 % |
≥40
|
≥42
|
|
≥45 |
≥53 |
≥53 |
≥53 |
≥57 |
≥55 |
≥62 |
≥58 |
≥60 |
Fe2O3 % |
≤2.0 |
≤1.6
|
|
≤1.7 |
|
|
|
|
|
|
|
|
SiC % |
|
|
|
|
≥7 |
≥5 |
≥11.5 |
|
|
|
≥10 |
≥10 |
C % |
|
|
|
|
≥10 |
≥11.5 |
≥5 |
≥6 |
≥8 |
≥4 |
≥8 |
≥8 |
SiC+ C % |
|
|
|
|
|
|
|
≥14 |
≥17 |
≥10 |
|
|
Al2O3+ SiC % |
|
|
|
|
≥65 |
≥65 |
≥65 |
|
|
|
|
|
耐火度 ℃
|
≥1730
|
≥1750
|
|
|
|
|
|
|
|
|
|
|
顯氣孔率 %
|
≤15
|
≤15 |
≤24 |
≤17 |
≤8.5 |
≤8.5 |
≤10 |
≤10 |
≤8 |
≤10 |
≤10 |
≤8 |
體積密度 g/cm3
|
≥2.30
|
|
|
|
≥2.75 |
≥2.75 |
≥2.75 |
≥2.75 |
≥2.75 |
≥2.75 |
≥2.75 |
≥2.85 |
常溫耐壓強(qiáng)度 Mpa
|
≥49.0 |
≥58.8 |
≥24.5 |
≥40 |
≥40 |
≥40 |
≥40 |
≥40 |
≥35 |
≥45 |
≥50 |
≥50 |
常溫抗折強(qiáng)度 MPa |
|
|
|
|
|
|
|
|
|
|
≥15 |
≥15 |
高溫抗折強(qiáng)度 Mpa |
|
|
|
|
|
|
|
1400℃ ×0.5h ≥5.5 |
1400℃ ×0.5h ≥5 |
1400℃ ×0.5h ≥6 |
1450℃ 保護(hù)≥5 |
1450℃ 保護(hù)≥8 |
荷重軟化溫度 ℃ |
T2≥1500 |
KD≥1450 |
|
|
|
|
|
|
|
|
|
|
重?zé)變化率 % |
|
1450 ℃×3h 0~-0.2 |
1400 ℃×2h +0.1~-0.5 |
1450 ℃×3h +0.1~-0.3 |
|
|
|
|
|
|
1450 ℃×2h 0~0.5 |
1400 ℃×2h 0~0.7 |
熱震穩(wěn)定性,次(1100℃ 水冷) |
≥10 無剝落 |
|
|
|
|
|
|
|
|
|
|
|
使用部位 |
工作層 永久層 |
混鐵車 工作層
|
混鐵車 永久層
|
鐵水罐 工作層 |
混鐵車 鐵水部 |
混鐵車 渣線部 |
混鐵車 頂部 |
混鐵車 鐵水部 |
混鐵車 渣線部 |
混鐵車 頂部
|
混鐵車 直筒部 |
混鐵車 錐體段 | | | |
|
【返回】 【關(guān)閉】 |
|
|
|
|